dyeing%cationic dyes%polysulfonamide fiber
以较小配伍值的阳离子染料对芳砜纶纤维进行载体染色,优化染色工艺为:阳离子染料0.5%owf,促染剂NaCl 50 g/L,载体MS 40 g/L,非离子渗透剂1 g/L,pH值3,浴比1:12,染色温度135℃,时间60 min.采用阳离子染料染色的芳砜纶纤维色牢度较好,均在4级左右.
以較小配伍值的暘離子染料對芳砜綸纖維進行載體染色,優化染色工藝為:暘離子染料0.5%owf,促染劑NaCl 50 g/L,載體MS 40 g/L,非離子滲透劑1 g/L,pH值3,浴比1:12,染色溫度135℃,時間60 min.採用暘離子染料染色的芳砜綸纖維色牢度較好,均在4級左右.
이교소배오치적양리자염료대방풍륜섬유진행재체염색,우화염색공예위:양리자염료0.5%owf,촉염제NaCl 50 g/L,재체MS 40 g/L,비리자삼투제1 g/L,pH치3,욕비1:12,염색온도135℃,시간60 min.채용양리자염료염색적방풍륜섬유색뇌도교호,균재4급좌우.
Carrier dyeing of polysutfonamide fiber was carried out with selected cationic dyes which had small compatible values.Optimum process was deined as follows:cationic dye 0.5% owf,a promoter NaCl 50 g/L,carrier MS 40 g/L,non-ionic penetrating agent 1 g/L,pH value 3,ratio 1:12,dyeing at 135℃ for 60 minutes.The dyeings featured 4-level color fastness.