云南某铜铅锌多金属硫化矿石铜、铅、锌含量分别为0. 58%、0. 75%、3. 01%,有害元素砷含量低. 为开发利用该矿石,对其进行了选矿试验研究. 结果表明:在磨矿细度为-0. 074 mm占85%条件下,以硫代硫酸钠、腐殖酸钠、六偏磷酸钠为脉石抑制剂、硫酸锌为锌矿物抑制剂、乙基黄药为捕收剂进行铜铅混合优先浮选,铜铅混合精矿以石灰为pH调整剂、EMY-306为抑制剂、Z-200为捕收剂进行铜铅分离,铜铅混浮尾矿以硫酸铜为活化剂、丁基黄药为捕收剂进行锌浮选,获得的铜精矿铜品位为26. 09%、回收率为71. 25%,铅精矿铅品位为48. 82%、回收率为69. 21%,锌精矿锌品位为49. 80%、回收率为87. 78%. 试验取得了较好的分选指标,为该矿石资源的开发利用提供了技术依据.
雲南某銅鉛鋅多金屬硫化礦石銅、鉛、鋅含量分彆為0. 58%、0. 75%、3. 01%,有害元素砷含量低. 為開髮利用該礦石,對其進行瞭選礦試驗研究. 結果錶明:在磨礦細度為-0. 074 mm佔85%條件下,以硫代硫痠鈉、腐殖痠鈉、六偏燐痠鈉為脈石抑製劑、硫痠鋅為鋅礦物抑製劑、乙基黃藥為捕收劑進行銅鉛混閤優先浮選,銅鉛混閤精礦以石灰為pH調整劑、EMY-306為抑製劑、Z-200為捕收劑進行銅鉛分離,銅鉛混浮尾礦以硫痠銅為活化劑、丁基黃藥為捕收劑進行鋅浮選,穫得的銅精礦銅品位為26. 09%、迴收率為71. 25%,鉛精礦鉛品位為48. 82%、迴收率為69. 21%,鋅精礦鋅品位為49. 80%、迴收率為87. 78%. 試驗取得瞭較好的分選指標,為該礦石資源的開髮利用提供瞭技術依據.
운남모동연자다금속류화광석동、연、자함량분별위0. 58%、0. 75%、3. 01%,유해원소신함량저. 위개발이용해광석,대기진행료선광시험연구. 결과표명:재마광세도위-0. 074 mm점85%조건하,이류대류산납、부식산납、륙편린산납위맥석억제제、류산자위자광물억제제、을기황약위포수제진행동연혼합우선부선,동연혼합정광이석회위pH조정제、EMY-306위억제제、Z-200위포수제진행동연분리,동연혼부미광이류산동위활화제、정기황약위포수제진행자부선,획득적동정광동품위위26. 09%、회수솔위71. 25%,연정광연품위위48. 82%、회수솔위69. 21%,자정광자품위위49. 80%、회수솔위87. 78%. 시험취득료교호적분선지표,위해광석자원적개발이용제공료기술의거.
There is 0. 58% copper,0. 75% lead,and 3. 01% zinc in a poly-metallic sulfide ore from Yunnan,with low content of harmful element arsenic. Beneficiation experiments were conducted on the ore to develop and utilize the ore. The re-sults indicated that,at the grinding fineness of 85% passing 0. 074 mm,with sodium thiosulfate,sodium hexametaphosphate, and humic acid as gangue inhibitors,sulfide zinc sulphate as zinc mineral inhibitor,and ethyl xanthate as collector via copper and lead bulk preference flotation,separation of copper from lead for bulk concentrate using slime as pH modifiers,EMY-306 as gangue inhibitors,Z-200 as collector,zinc flotation using copper sulfate as the activator,butyl xanthate as collector,copper concentrate with 26. 09% Cu and recovery of 71. 25%,lead concentrate with 48. 82% Pb and recovery of 69. 21%,and zinc concentrate with 49. 80% Zn and recovery of 87. 78% are obtained respectively. Good beneficiation test results had been ob-tained,which provide technique basis for reasonably recovery of the resource.